POM, HIPS, HPVC, PMMA, SAN, ABS, PP, PU, HDPE, PBT, PBT Glass Fiber, PA6, ABS+PC, PBT+GF, PA6+GF, PC & PEEK are the plastic materials that we commonly use for making mold and making plastic injection molding production job for customer.  
POM, HIPS, HPVC, PMMA, SAN, ABS, PP, PU, HDPE, PBT, PBT Glass Fiber, PA6, ABS+PC, PBT+GF, PA6+GF, PC & PEEK are the plastic materials that we commonly use for making mold and making plastic injection molding production job for customer.  

Material, Machine & Mold Temperature information 

POM, HIPS, HPVC, PMMA, SAN, ABS, PP, PU, HDPE, PBT, PBT Glass Fiber, PA6, ABS+PC, PBT+GF, PA6+GF, PC & PEEK are the plastic materials that we commonly use for making mold and making plastic injection molding production job for customer.  
 
In this chart, you may easily know all the machine temperature, mold temperature, raw material baking hours and raw material dry temperature information suggested for each differnt plastics molding conidition.  
 
Intertech has good experience in running all these material's mold making and molding production job for long time.  Welcome to contact us for your need !
 
Plastics we commonly use Injection Machine Screw temperature Suggested. Mold Temperature Suggested. Raw Materail baking hour Material dry temperature
POM 160-280 10-80 2~3 60-70
HIPS 170-250 10-80 2~4 60-80
HPVC 180-210 30-50 2~3 40-70
PMMA 180-260 50-80 3~5 70-80
SAN 180-270 40-80 2~4 70-80
ABS 180-250 50-90 2~3 80-90
PP 190-270 30-80 2~3 40-80
PU 195-230 20-40 2~3 80-90
HDPE 200-260 30-70    
PBT 220-260 50-100 3~4 120-140
PBT Glass Fiber 230-270 80-110 3~4 120-140
PA6 230-260 60-90 4~6 75-90
ABS+PC 240-290 90-110 2~4 100-120
PBT+GF 250-270 60-100 3~4 120-140
PA66 260-290 60-100 3~5 75-90
PET 260-290 120-140 2~4 120-160
PP+GF 260-280 50-80 2~3 40-90
PA6+GF 270-300 70-120 4~6 75-80
PC 280-320 80-100 2~4 110-120
PEEK 340-390 120-150 2~4 140-150